3003 (3.0517, A93003) Aluminum
Material Properties
Base Metal Price: 9.6 % rel
Density: 2.73 g/cm3 (170 lb/ft3)
Elastic (Young's, Tensile) Modulus: 69 GPa (10.0 x 106 psi)
Electrical Conductivity: 40 to 50 % IACS
Elongation at Break: 4 to 38 %
Melting Onset (Solidus): 643 °C (1190 °F)
Poisson's Ratio: 0.33
Shear Modulus: 25 GPa (3.6 106 psi)
Specific Heat Capacity: 900 J/kg-K
Tensile Strength: Ultimate (UTS): 110 to 200 MPa (16 to 29 x 103 psi)
Tensile Strength: Yield (Proof): 40 to 190 MPa (5.8 to 28 x 103 psi)
Thermal Conductivity: 160 to 190 W/m-K
Thermal Expansion: 23.2 µm/m-K
Alloy Composition
Aluminum (Al): 96.8 to 99 %
Manganese (Mn): 1.0 to 1.5 %
Iron (Fe): 0 to 0.7 %
Silicon (Si): 0 to 0.6 %
Copper (Cu): 0.05 to 0.20 %
Residuals: 0 to 0.15 %
Zinc (Zn): 0 to 0.1 %
See Also
Aluminum Standards and Data, Aluminum Association Inc., 2013
ASTM B 209: Standard Specification for Aluminum and Aluminum-Alloy Sheet and Plate
ASTM B 210: Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes
ASTM B 211: Standard Specification for Aluminum and Aluminum-Alloy Bar, Rod, and Wire
ASTM B 221: Standard Specification for Aluminum and Aluminum-Alloy Extruded Bars, Rods, Wire, Profiles, and Tubes
ASTM B 483: Standard Specification for Aluminum and Aluminum-Alloy Drawn Tube and Pipe for General Purpose Applications
ASTM B 491: Standard Specification for Aluminum and Aluminum-Alloy Extruded Round Tubes for General-Purpose Applications
ASTM B 547: Standard Specification for Aluminum and Aluminum-Alloy Formed and Arc-Welded Round Tube
ISO 6361: Wrought Aluminium and Aluminium Alloy Sheets, Strips and Plates