ASTM A216 Cast Steel vs. Automotive Malleable Cast Iron

Both ASTM A216 cast steel and automotive malleable cast iron are iron alloys. There are 27 material properties with values for both materials. Properties with values for just one material (4, in this case) are not shown.

For each property being compared, the top bar is ASTM A216 cast steel and the bottom bar is automotive malleable cast iron.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 190
180
Elongation at Break, % 25 to 27
1.0 to 10
Poisson's Ratio 0.29
0.29
Shear Modulus, GPa 72
70
Tensile Strength: Ultimate (UTS), MPa 500 to 570
350 to 720
Tensile Strength: Yield (Proof), MPa 230 to 310
220 to 590

Thermal Properties

Latent Heat of Fusion, J/g 250
260
Melting Completion (Liquidus), °C 1450 to 1460
1410
Melting Onset (Solidus), °C 1410
1370
Specific Heat Capacity, J/kg-K 470
480
Thermal Conductivity, W/m-K 49 to 52
41
Thermal Expansion, µm/m-K 12
14

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 7.1 to 7.2
7.4
Electrical Conductivity: Equal Weight (Specific), % IACS 8.2 to 8.3
8.7

Otherwise Unclassified Properties

Base Metal Price, % relative 1.8
1.9
Density, g/cm3 7.8
7.6
Embodied Carbon, kg CO2/kg material 1.4
1.5
Embodied Energy, MJ/kg 18
20
Embodied Water, L/kg 45
45

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 110 to 120
6.8 to 30
Resilience: Unit (Modulus of Resilience), kJ/m3 140 to 250
130 to 950
Stiffness to Weight: Axial, points 13
13
Stiffness to Weight: Bending, points 24
25
Strength to Weight: Axial, points 18 to 20
13 to 26
Strength to Weight: Bending, points 18 to 20
14 to 24
Thermal Diffusivity, mm2/s 13 to 14
11
Thermal Shock Resistance, points 16 to 18
9.9 to 21