Metric UnitsUS Customary Units
Mechanical Properties
| Elastic (Young's, Tensile) Modulus, GPa | 2.6 | |
| 1.9 to 2.9 |
| Elongation at Break, % | 6.0 | |
| 1.8 to 40 |
| Tensile Strength: Ultimate (UTS), MPa | 55 | |
| 32 to 44 |
Thermal Properties
| Glass Transition Temperature, °C | 100 | |
| 100 |
| Specific Heat Capacity, J/kg-K | 1300 | |
| 1250 to 1400 |
| Thermal Conductivity, W/m-K | 0.18 | |
| 0.14 to 0.22 |
| Thermal Expansion, µm/m-K | 95 | |
| 80 to 98 |
| Vicat Softening Temperature, °C | 96 | |
| 100 to 110 |
Electrical Properties
| Electrical Resistivity Order of Magnitude, 10x Ω-m | 13 | |
| 14 to 15 |
Otherwise Unclassified Properties
| Density, g/cm3 | 1.1 | |
| 1.0 |
Common Calculations
| Stiffness to Weight: Axial, points | 1.3 | |
| 1.0 to 1.5 |
| Stiffness to Weight: Bending, points | 43 | |
| 40 to 45 |
| Strength to Weight: Axial, points | 14 | |
| 8.5 to 12 |
| Strength to Weight: Bending, points | 30 | |
| 22 to 26 |
| Thermal Diffusivity, mm2/s | 0.13 | |
| 0.11 to 0.15 |
| Thermal Shock Resistance, points | 16 | |
| 11 to 15 |