Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 220
190
Elongation at Break, % 34
17 to 18
Fatigue Strength, MPa 260
240
Poisson's Ratio 0.29
0.29
Shear Modulus, GPa 84
73
Tensile Strength: Ultimate (UTS), MPa 620
590 to 670
Tensile Strength: Yield (Proof), MPa 350
350 to 360

Thermal Properties

Latent Heat of Fusion, J/g 330
260
Maximum Temperature: Mechanical, °C 980
410
Melting Completion (Liquidus), °C 1550
1450
Melting Onset (Solidus), °C 1490
1410
Specific Heat Capacity, J/kg-K 430
470
Thermal Conductivity, W/m-K 10
52
Thermal Expansion, µm/m-K 12
13

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 1.5
7.3
Electrical Conductivity: Equal Weight (Specific), % IACS 1.5
8.4

Otherwise Unclassified Properties

Base Metal Price, % relative 65
2.1
Density, g/cm3 8.9
7.8
Embodied Carbon, kg CO2/kg material 12
1.4
Embodied Energy, MJ/kg 170
19
Embodied Water, L/kg 290
49

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 180
93 to 96
Resilience: Unit (Modulus of Resilience), kJ/m3 290
330 to 350
Stiffness to Weight: Axial, points 14
13
Stiffness to Weight: Bending, points 23
24
Strength to Weight: Axial, points 19
21 to 24
Strength to Weight: Bending, points 18
20 to 22
Thermal Diffusivity, mm2/s 2.7
14
Thermal Shock Resistance, points 17
17 to 20