Titanium 4-4-2 belongs to the titanium alloys classification, while ASTM A732 cast steel belongs to the iron alloys. There are 27 material properties with values for both materials. Properties with values for just one material (5, in this case) are not shown.

For each property being compared, the top bar is titanium 4-4-2 and the bottom bar is ASTM A732 cast steel.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 110
190
Elongation at Break, % 10
4.0 to 25
Fatigue Strength, MPa 590 to 620
230 to 750
Poisson's Ratio 0.32
0.29
Shear Modulus, GPa 42
72 to 73
Tensile Strength: Ultimate (UTS), MPa 1150 to 1250
460 to 1470
Tensile Strength: Yield (Proof), MPa 1030 to 1080
310 to 1340

Thermal Properties

Latent Heat of Fusion, J/g 410
250 to 260
Maximum Temperature: Mechanical, °C 310
400 to 430
Melting Completion (Liquidus), °C 1610
1440 to 1460
Melting Onset (Solidus), °C 1560
1400 to 1420
Specific Heat Capacity, J/kg-K 540
470 to 480
Thermal Conductivity, W/m-K 6.7
39 to 50
Thermal Expansion, µm/m-K 8.6
13

Otherwise Unclassified Properties

Base Metal Price, % relative 39
2.0 to 3.8
Density, g/cm3 4.7
7.8 to 7.9
Embodied Carbon, kg CO2/kg material 30
1.4 to 1.7
Embodied Energy, MJ/kg 480
19 to 24
Embodied Water, L/kg 180
47 to 54

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 110 to 120
45 to 130
Resilience: Unit (Modulus of Resilience), kJ/m3 4700 to 5160
260 to 4770
Stiffness to Weight: Axial, points 13
13
Stiffness to Weight: Bending, points 34
24
Strength to Weight: Axial, points 68 to 74
16 to 52
Strength to Weight: Bending, points 52 to 55
17 to 37
Thermal Diffusivity, mm2/s 2.6
10 to 14
Thermal Shock Resistance, points 86 to 93
14 to 43