Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 120
110
Poisson's Ratio 0.32
0.33
Rockwell B Hardness 63 to 93
46 to 85
Rockwell Superficial 30T Hardness 58 to 78
51 to 77
Shear Modulus, GPa 47
42
Tensile Strength: Ultimate (UTS), MPa 400 to 660
330 to 570

Thermal Properties

Latent Heat of Fusion, J/g 210
200
Maximum Temperature: Mechanical, °C 200
170
Melting Completion (Liquidus), °C 1110
1040
Melting Onset (Solidus), °C 1070
1000
Specific Heat Capacity, J/kg-K 400
390
Thermal Conductivity, W/m-K 33
170
Thermal Expansion, µm/m-K 18
18

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 6.0
40
Electrical Conductivity: Equal Weight (Specific), % IACS 6.3
42

Otherwise Unclassified Properties

Base Metal Price, % relative 33
28
Density, g/cm3 8.5
8.7
Embodied Carbon, kg CO2/kg material 4.1
2.6
Embodied Energy, MJ/kg 62
42
Embodied Water, L/kg 300
310

Common Calculations

Stiffness to Weight: Axial, points 8.0
7.2
Stiffness to Weight: Bending, points 19
19
Strength to Weight: Axial, points 13 to 21
11 to 18
Strength to Weight: Bending, points 14 to 20
12 to 18
Thermal Diffusivity, mm2/s 9.8
52
Thermal Shock Resistance, points 13 to 22
11 to 19

Alloy Composition


Deprecated: Automatic conversion of false to array is deprecated in /home/public/compare.php on line 452
Copper (Cu), % 63.5 to 66.5
86 to 89
Iron (Fe), % 0 to 0.25
0 to 0.050
Lead (Pb), % 0 to 0.050
0 to 0.050
Manganese (Mn), % 0 to 0.5
0
Nickel (Ni), % 16.5 to 19.5
0
Zinc (Zn), % 12.7 to 20
10.7 to 14
Residuals, % 0 to 0.5
0 to 0.2