1/16-Hard 201LN Stainless Steel
1/16-hard AISI 201LN is AISI 201LN stainless steel in the 1/16-hard temper. It has the second lowest strength and second highest ductility compared to the other variants of AISI 201LN stainless steel.
The graph bars on the material properties cards below compare 1/16-hard AISI 201LN to: wrought austenitic stainless steels (top), all iron alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Brinell Hardness
230
Elastic (Young's, Tensile) Modulus
200 GPa 29 x 106 psi
Elongation at Break
45 %
Fatigue Strength
360 MPa 52 x 103 psi
Poisson's Ratio
0.28
Shear Modulus
77 GPa 11 x 106 psi
Shear Strength
540 MPa 78 x 103 psi
Tensile Strength: Ultimate (UTS)
770 MPa 110 x 103 psi
Tensile Strength: Yield (Proof)
390 MPa 57 x 103 psi
Thermal Properties
Latent Heat of Fusion
280 J/g
Maximum Temperature: Corrosion
410 °C 770 °F
Maximum Temperature: Mechanical
880 °C 1610 °F
Melting Completion (Liquidus)
1410 °C 2570 °F
Melting Onset (Solidus)
1370 °C 2490 °F
Specific Heat Capacity
480 J/kg-K 0.11 BTU/lb-°F
Thermal Conductivity
15 W/m-K 8.7 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
2.4 % IACS
Electrical Conductivity: Equal Weight (Specific)
2.9 % IACS
Otherwise Unclassified Properties
Base Metal Price
12 % relative
Density
7.7 g/cm3 480 lb/ft3
Embodied Carbon
2.6 kg CO2/kg material
Embodied Energy
38 MJ/kg 16 x 103 BTU/lb
Embodied Water
140 L/kg 17 gal/lb
Common Calculations
PREN (Pitting Resistance)
20
Resilience: Ultimate (Unit Rupture Work)
290 MJ/m3
Resilience: Unit (Modulus of Resilience)
390 kJ/m3
Stiffness to Weight: Axial
14 points
Stiffness to Weight: Bending
25 points
Strength to Weight: Axial
28 points
Strength to Weight: Bending
24 points
Thermal Diffusivity
4.0 mm2/s
Thermal Shock Resistance
17 points
Alloy Composition
| Fe | 67.9 to 73.5 | |
| Cr | 16 to 17.5 | |
| Mn | 6.4 to 7.5 | |
| Ni | 4.0 to 5.0 | |
| Cu | 0 to 1.0 | |
| Si | 0 to 0.75 | |
| N | 0.1 to 0.25 | |
| P | 0 to 0.045 | |
| C | 0 to 0.030 | |
| S | 0 to 0.015 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM A666: Standard Specification for Annealed or Cold-Worked Austenitic Stainless Steel Sheet, Strip, Plate, and Flat Bar
Welding Metallurgy of Stainless Steels, Erich Folkhard et al., 2012
ASTM A959: Standard Guide for Specifying Harmonized Standard Grade Compositions for Wrought Stainless Steels
Corrosion of Austenitic Stainless Steels: Mechanism, Mitigation and Monitoring, H. S. Khatak and B. Raj (editors), 2002
Austenitic Stainless Steels: Microstructure and Mechanical Properties, P. Marshall, 1984