2030-T3511 Aluminum
2030-T3511 aluminum is 2030 aluminum in the T3511 temper. To achieve this temper, the metal is solution heat-treated, stress relieved, then naturally aged. The stress relief is accomplished by stretching the metal by an amount that depends on the type of standard wrought product being made (extrusion or tube). The metal is straightened after the stretching operation. This temper is closely related to T3510, which does not permit such straightening.
The graph bars on the material properties cards below compare 2030-T3511 aluminum to: 2000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
70 GPa 10 x 106 psi
Elongation at Break
5.6 %
Fatigue Strength
97 MPa 14 x 103 psi
Poisson's Ratio
0.33
Shear Modulus
26 GPa 3.8 x 106 psi
Shear Strength
240 MPa 35 x 103 psi
Tensile Strength: Ultimate (UTS)
410 MPa 60 x 103 psi
Tensile Strength: Yield (Proof)
270 MPa 40 x 103 psi
Thermal Properties
Latent Heat of Fusion
390 J/g
Maximum Temperature: Mechanical
190 °C 380 °F
Melting Completion (Liquidus)
640 °C 1180 °F
Melting Onset (Solidus)
510 °C 950 °F
Specific Heat Capacity
870 J/kg-K 0.21 BTU/lb-°F
Thermal Conductivity
130 W/m-K 77 BTU/h-ft-°F
Thermal Expansion
23 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
34 % IACS
Electrical Conductivity: Equal Weight (Specific)
99 % IACS
Otherwise Unclassified Properties
Base Metal Price
10 % relative
Density
3.1 g/cm3 190 lb/ft3
Embodied Carbon
8.0 kg CO2/kg material
Embodied Energy
150 MJ/kg 63 x 103 BTU/lb
Embodied Water
1140 L/kg 140 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
21 MJ/m3
Resilience: Unit (Modulus of Resilience)
530 kJ/m3
Stiffness to Weight: Axial
13 points
Stiffness to Weight: Bending
45 points
Strength to Weight: Axial
37 points
Strength to Weight: Bending
40 points
Thermal Diffusivity
50 mm2/s
Thermal Shock Resistance
18 points
Alloy Composition
| Al | 88.9 to 95.2 | |
| Cu | 3.3 to 4.5 | |
| Pb | 0.8 to 1.5 | |
| Mg | 0.5 to 1.3 | |
| Mn | 0.2 to 1.0 | |
| Si | 0 to 0.8 | |
| Fe | 0 to 0.7 | |
| Zn | 0 to 0.5 | |
| Ti | 0 to 0.2 | |
| Bi | 0 to 0.2 | |
| Cr | 0 to 0.1 | |
| res. | 0 to 0.3 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
Aerospace Materials, Brian Cantor et al. (editors), 2001
EN 754-2: Aluminium and aluminium alloys. Cold drawn rod/bar and tube. Mechanical properties
ASM Specialty Handbook: Aluminum and Aluminum Alloys, J. R. Davis (editor), 1993
EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products