5082-H19 Aluminum
5082-H19 aluminum is 5082 aluminum in the H19 temper. To achieve this temper, the metal is strain hardened to a strength that exceeds H18 by at least 10 MPa (or 1.5 ksi). The graph bars on the material properties cards below compare 5082-H19 aluminum to: 5000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
67 GPa 9.8 x 106 psi
Elongation at Break
1.1 %
Fatigue Strength
110 MPa 15 x 103 psi
Poisson's Ratio
0.33
Shear Modulus
25 GPa 3.7 x 106 psi
Shear Strength
230 MPa 33 x 103 psi
Tensile Strength: Ultimate (UTS)
400 MPa 58 x 103 psi
Tensile Strength: Yield (Proof)
340 MPa 50 x 103 psi
Thermal Properties
Latent Heat of Fusion
400 J/g
Maximum Temperature: Mechanical
180 °C 360 °F
Melting Completion (Liquidus)
640 °C 1190 °F
Melting Onset (Solidus)
560 °C 1040 °F
Specific Heat Capacity
910 J/kg-K 0.22 BTU/lb-°F
Thermal Conductivity
130 W/m-K 76 BTU/h-ft-°F
Thermal Expansion
24 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
32 % IACS
Electrical Conductivity: Equal Weight (Specific)
110 % IACS
Otherwise Unclassified Properties
Base Metal Price
9.5 % relative
Density
2.7 g/cm3 170 lb/ft3
Embodied Carbon
8.9 kg CO2/kg material
Embodied Energy
150 MJ/kg 66 x 103 BTU/lb
Embodied Water
1180 L/kg 140 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
4.3 MJ/m3
Resilience: Unit (Modulus of Resilience)
870 kJ/m3
Stiffness to Weight: Axial
14 points
Stiffness to Weight: Bending
51 points
Strength to Weight: Axial
41 points
Strength to Weight: Bending
45 points
Thermal Diffusivity
54 mm2/s
Thermal Shock Resistance
18 points
Alloy Composition
| Al | 93.5 to 96 | |
| Mg | 4.0 to 5.0 | |
| Fe | 0 to 0.35 | |
| Zn | 0 to 0.25 | |
| Si | 0 to 0.2 | |
| Mn | 0 to 0.15 | |
| Cr | 0 to 0.15 | |
| Cu | 0 to 0.15 | |
| Ti | 0 to 0.1 | |
| res. | 0 to 0.15 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
Handbook of Aluminum Bonding Technology and Data, J. D. Minford, 1993
ASM Specialty Handbook: Aluminum and Aluminum Alloys, J. R. Davis (editor), 1993
ISO 6361-2: Wrought aluminium and aluminium alloys - Sheets, strips and plates - Part 2: Mechanical properties
EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products