Annealed (A or TB00) C17000 Copper
TB00 C17000 copper is C17000 copper in the TB00 (solution heat treated) temper. It has the lowest strength and highest ductility compared to the other variants of C17000 copper. The graph bars on the material properties cards below compare TB00 C17000 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
31 %
Poisson's Ratio
0.33
Rockwell B Hardness
63
Rockwell Superficial 30T Hardness
57
Shear Modulus
45 GPa 6.5 x 106 psi
Shear Strength
320 MPa 47 x 103 psi
Tensile Strength: Ultimate (UTS)
490 MPa 71 x 103 psi
Tensile Strength: Yield (Proof)
160 MPa 23 x 103 psi
Thermal Properties
Latent Heat of Fusion
230 J/g
Maximum Temperature: Mechanical
270 °C 510 °F
Melting Completion (Liquidus)
980 °C 1800 °F
Melting Onset (Solidus)
870 °C 1590 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
110 W/m-K 62 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
22 % IACS
Electrical Conductivity: Equal Weight (Specific)
22 % IACS
Otherwise Unclassified Properties
Density
8.8 g/cm3 550 lb/ft3
Embodied Carbon
8.7 kg CO2/kg material
Embodied Energy
140 MJ/kg 58 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
120 MJ/m3
Resilience: Unit (Modulus of Resilience)
110 kJ/m3
Stiffness to Weight: Axial
7.6 points
Stiffness to Weight: Bending
19 points
Strength to Weight: Axial
15 points
Strength to Weight: Bending
16 points
Thermal Diffusivity
32 mm2/s
Thermal Shock Resistance
17 points
Alloy Composition
| Cu | 96.3 to 98.2 | |
| Be | 1.6 to 1.8 | |
| Ni | 0.2 to 0.6 | |
| Fe | 0 to 0.4 | |
| Si | 0 to 0.2 | |
| Al | 0 to 0.2 | |
| res. | 0 to 0.5 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B196: Standard Specification for Copper-Beryllium Alloy Rod and Bar
ASTM B194: Standard Specification for Copper-Beryllium Alloy Plate, Sheet, Strip, and Rolled Bar
Copper Alloys: Preparation, Properties and Applications, Michael Naboka and Jennifer Giordano (editors), 2013
ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001
CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015