Annealed and Aged (AT or TF00) C17200 Copper
TF00 C17200 copper is C17200 copper in the TF00 (precipitation hardened) temper. The graph bars on the material properties cards below compare TF00 C17200 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
5.6 %
Fatigue Strength
290 MPa 42 x 103 psi
Poisson's Ratio
0.33
Rockwell C Hardness
40
Shear Modulus
45 GPa 6.5 x 106 psi
Shear Strength
730 MPa 110 x 103 psi
Tensile Strength: Ultimate (UTS)
1250 MPa 180 x 103 psi
Tensile Strength: Yield (Proof)
1110 MPa 160 x 103 psi
Thermal Properties
Latent Heat of Fusion
230 J/g
Maximum Temperature: Mechanical
280 °C 530 °F
Melting Completion (Liquidus)
980 °C 1800 °F
Melting Onset (Solidus)
870 °C 1590 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
110 W/m-K 61 BTU/h-ft-°F
Thermal Expansion
18 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
22 % IACS
Electrical Conductivity: Equal Weight (Specific)
23 % IACS
Otherwise Unclassified Properties
Density
8.8 g/cm3 550 lb/ft3
Embodied Carbon
9.4 kg CO2/kg material
Embodied Energy
150 MJ/kg 63 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
68 MJ/m3
Resilience: Unit (Modulus of Resilience)
5080 kJ/m3
Stiffness to Weight: Axial
7.6 points
Stiffness to Weight: Bending
19 points
Strength to Weight: Axial
39 points
Strength to Weight: Bending
29 points
Thermal Diffusivity
31 mm2/s
Thermal Shock Resistance
42 points
Alloy Composition
| Cu | 96.1 to 98 | |
| Be | 1.8 to 2.0 | |
| Ni | 0.2 to 0.6 | |
| Fe | 0 to 0.4 | |
| Si | 0 to 0.2 | |
| Al | 0 to 0.2 | |
| res. | 0 to 0.5 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B196: Standard Specification for Copper-Beryllium Alloy Rod and Bar
ASTM B194: Standard Specification for Copper-Beryllium Alloy Plate, Sheet, Strip, and Rolled Bar
Copper: Its Trade, Manufacture, Use, and Environmental Status, Gunter Joseph, 2001
Properties and Selection: Nonferrous Alloys and Special-Purpose Materials, ASM Handbook vol. 2, ASM International, 1993