Full-Hard (H04) C15100 Copper
H04 C15100 copper is C15100 copper in the H04 (full hard) temper. The graph bars on the material properties cards below compare H04 C15100 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
4.0 %
Poisson's Ratio
0.34
Rockwell B Hardness
57
Rockwell F Hardness
59
Rockwell Superficial 30T Hardness
61
Shear Modulus
43 GPa 6.3 x 106 psi
Shear Strength
230 MPa 33 x 103 psi
Tensile Strength: Ultimate (UTS)
390 MPa 57 x 103 psi
Tensile Strength: Yield (Proof)
380 MPa 55 x 103 psi
Thermal Properties
Latent Heat of Fusion
210 J/g
Maximum Temperature: Mechanical
200 °C 390 °F
Melting Completion (Liquidus)
1100 °C 2010 °F
Melting Onset (Solidus)
1030 °C 1890 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
360 W/m-K 210 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
95 % IACS
Electrical Conductivity: Equal Weight (Specific)
95 % IACS
Otherwise Unclassified Properties
Base Metal Price
31 % relative
Density
9.0 g/cm3 560 lb/ft3
Embodied Carbon
2.7 kg CO2/kg material
Embodied Energy
43 MJ/kg 18 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
16 MJ/m3
Resilience: Unit (Modulus of Resilience)
620 kJ/m3
Stiffness to Weight: Axial
7.2 points
Stiffness to Weight: Bending
18 points
Strength to Weight: Axial
12 points
Strength to Weight: Bending
13 points
Thermal Diffusivity
100 mm2/s
Thermal Shock Resistance
14 points
Alloy Composition
| Cu | 99.8 to 99.95 | |
| Zr | 0.050 to 0.15 | |
| res. | 0 to 0.1 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
Copper Alloys: Preparation, Properties and Applications, Michael Naboka and Jennifer Giordano (editors), 2013