Full-Hard (H04) C65100 Bronze
H04 C65100 bronze is C65100 bronze in the H04 (full hard) temper. The graph bars on the material properties cards below compare H04 C65100 bronze to: wrought bronzes (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
12 %
Fatigue Strength
170 MPa 25 x 103 psi
Poisson's Ratio
0.34
Rockwell B Hardness
79
Shear Modulus
43 GPa 6.3 x 106 psi
Shear Strength
310 MPa 45 x 103 psi
Tensile Strength: Ultimate (UTS)
480 MPa 70 x 103 psi
Tensile Strength: Yield (Proof)
330 MPa 47 x 103 psi
Thermal Properties
Latent Heat of Fusion
230 J/g
Maximum Temperature: Mechanical
200 °C 390 °F
Melting Completion (Liquidus)
1060 °C 1940 °F
Melting Onset (Solidus)
1030 °C 1890 °F
Specific Heat Capacity
390 J/kg-K 0.094 BTU/lb-°F
Thermal Conductivity
57 W/m-K 33 BTU/h-ft-°F
Thermal Expansion
18 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
12 % IACS
Electrical Conductivity: Equal Weight (Specific)
12 % IACS
Otherwise Unclassified Properties
Base Metal Price
30 % relative
Calomel Potential
-280 mV
Density
8.8 g/cm3 550 lb/ft3
Embodied Carbon
2.6 kg CO2/kg material
Embodied Energy
41 MJ/kg 18 x 103 BTU/lb
Embodied Water
300 L/kg 36 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
51 MJ/m3
Resilience: Unit (Modulus of Resilience)
460 kJ/m3
Stiffness to Weight: Axial
7.3 points
Stiffness to Weight: Bending
18 points
Strength to Weight: Axial
15 points
Strength to Weight: Bending
15 points
Thermal Diffusivity
16 mm2/s
Thermal Shock Resistance
17 points
Alloy Composition
| Cu | 94.5 to 99.2 | |
| Si | 0.8 to 2.0 | |
| Zn | 0 to 1.5 | |
| Fe | 0 to 0.8 | |
| Mn | 0 to 0.7 | |
| Pb | 0 to 0.050 | |
| res. | 0 to 0.5 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B98: Standard Specification for Copper-Silicon Alloy Rod, Bar and Shapes
ASTM B96: Standard Specification for Copper-Silicon Alloy Plate, Sheet, Strip, and Rolled Bar for General Purposes and Pressure Vessels
Copper: Its Trade, Manufacture, Use, and Environmental Status, Gunter Joseph, 2001
Pressure Vessels: External Pressure Technology, 2nd ed., Carl T. F. Ross, 2011
Properties and Selection: Nonferrous Alloys and Special-Purpose Materials, ASM Handbook vol. 2, ASM International, 1993