Hot Rolled (+U) 1.5535 Steel
EN 1.5535 +U steel is EN 1.5535 steel in the hot worked condition. It has the second lowest strength and highest ductility compared to the other variants of EN 1.5535 steel. The graph bars on the material properties cards below compare EN 1.5535 +U steel to: EN wrought alloy steels (top), all iron alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Brinell Hardness
160
Elastic (Young's, Tensile) Modulus
190 GPa 27 x 106 psi
Elongation at Break
22 %
Fatigue Strength
210 MPa 31 x 103 psi
Poisson's Ratio
0.29
Reduction in Area
67 %
Shear Modulus
73 GPa 11 x 106 psi
Shear Strength
330 MPa 47 x 103 psi
Tensile Strength: Ultimate (UTS)
520 MPa 75 x 103 psi
Tensile Strength: Yield (Proof)
300 MPa 44 x 103 psi
Thermal Properties
Latent Heat of Fusion
250 J/g
Maximum Temperature: Mechanical
400 °C 760 °F
Melting Completion (Liquidus)
1460 °C 2660 °F
Melting Onset (Solidus)
1420 °C 2590 °F
Specific Heat Capacity
470 J/kg-K 0.11 BTU/lb-°F
Thermal Conductivity
50 W/m-K 29 BTU/h-ft-°F
Thermal Expansion
13 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
7.2 % IACS
Electrical Conductivity: Equal Weight (Specific)
8.2 % IACS
Otherwise Unclassified Properties
Base Metal Price
1.9 % relative
Density
7.8 g/cm3 490 lb/ft3
Embodied Carbon
1.4 kg CO2/kg material
Embodied Energy
19 MJ/kg 8.0 x 103 BTU/lb
Embodied Water
48 L/kg 5.7 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
97 MJ/m3
Resilience: Unit (Modulus of Resilience)
240 kJ/m3
Stiffness to Weight: Axial
13 points
Stiffness to Weight: Bending
24 points
Strength to Weight: Axial
18 points
Strength to Weight: Bending
18 points
Thermal Diffusivity
13 mm2/s
Thermal Shock Resistance
15 points
Alloy Composition
| Fe | 97.6 to 98.9 | |
| Mn | 0.9 to 1.2 | |
| C | 0.2 to 0.25 | |
| Si | 0 to 0.3 | |
| Cr | 0 to 0.3 | |
| Cu | 0 to 0.25 | |
| P | 0 to 0.025 | |
| S | 0 to 0.025 | |
| B | 0.00080 to 0.0050 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
Boron in Steel, S. K. Banerji and J. E. Morral (editors), 1980
EN 10263-4: Steel rod, bars and wire for cold heading and cold extrusion - Part 4: Technical delivery conditions for steels for quenching and tempering
ASM Specialty Handbook: Carbon and Alloy Steels, J. R. Davis (editor), 1996
Manufacture and Uses of Alloy Steels, Henry D. Hibbard, 2005
Ferrous Materials: Steel and Cast Iron, Hans Berns and Werner Theisen, 2008
CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015
Steels: Processing, Structure, and Performance, 2nd ed., George Krauss, 2015