Quarter-Hard and Stress Relieved (HR01) C19000 Copper
HR01 C19000 copper is C19000 copper in the HR01 (quarter-hard and stress relieved) temper. The graph bars on the material properties cards below compare HR01 C19000 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
13 %
Poisson's Ratio
0.34
Shear Modulus
43 GPa 6.3 x 106 psi
Shear Strength
280 MPa 40 x 103 psi
Tensile Strength: Ultimate (UTS)
550 MPa 80 x 103 psi
Tensile Strength: Yield (Proof)
510 MPa 75 x 103 psi
Thermal Properties
Latent Heat of Fusion
210 J/g
Maximum Temperature: Mechanical
200 °C 390 °F
Melting Completion (Liquidus)
1080 °C 1980 °F
Melting Onset (Solidus)
1040 °C 1900 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
250 W/m-K 150 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
60 % IACS
Electrical Conductivity: Equal Weight (Specific)
61 % IACS
Otherwise Unclassified Properties
Base Metal Price
31 % relative
Density
8.9 g/cm3 560 lb/ft3
Embodied Carbon
2.7 kg CO2/kg material
Embodied Energy
42 MJ/kg 18 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
70 MJ/m3
Resilience: Unit (Modulus of Resilience)
1140 kJ/m3
Stiffness to Weight: Axial
7.2 points
Stiffness to Weight: Bending
18 points
Strength to Weight: Axial
17 points
Strength to Weight: Bending
17 points
Thermal Diffusivity
73 mm2/s
Thermal Shock Resistance
20 points
Alloy Composition
| Cu | 96.9 to 99 | |
| Ni | 0.9 to 1.3 | |
| Zn | 0 to 0.8 | |
| P | 0.15 to 0.35 | |
| Fe | 0 to 0.1 | |
| Pb | 0 to 0.050 | |
| res. | 0 to 0.5 |
All values are % weight. Ranges represent what is permitted under applicable standards.