TH02 Tempered C17000 Copper
TH02 C17000 copper is C17000 copper in the TH02 (half-hard and precipitation heat treated) temper. It has the second highest strength and lowest ductility compared to the other variants of C17000 copper. The graph bars on the material properties cards below compare TH02 C17000 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
1.1 %
Poisson's Ratio
0.33
Rockwell C Hardness
42
Shear Modulus
45 GPa 6.5 x 106 psi
Shear Strength
720 MPa 110 x 103 psi
Tensile Strength: Ultimate (UTS)
1280 MPa 180 x 103 psi
Tensile Strength: Yield (Proof)
1140 MPa 170 x 103 psi
Thermal Properties
Latent Heat of Fusion
230 J/g
Maximum Temperature: Mechanical
270 °C 510 °F
Melting Completion (Liquidus)
980 °C 1800 °F
Melting Onset (Solidus)
870 °C 1590 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
110 W/m-K 62 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
22 % IACS
Electrical Conductivity: Equal Weight (Specific)
22 % IACS
Otherwise Unclassified Properties
Density
8.8 g/cm3 550 lb/ft3
Embodied Carbon
8.7 kg CO2/kg material
Embodied Energy
140 MJ/kg 58 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
14 MJ/m3
Resilience: Unit (Modulus of Resilience)
5420 kJ/m3
Stiffness to Weight: Axial
7.6 points
Stiffness to Weight: Bending
19 points
Strength to Weight: Axial
40 points
Strength to Weight: Bending
30 points
Thermal Diffusivity
32 mm2/s
Thermal Shock Resistance
44 points
Alloy Composition
| Cu | 96.3 to 98.2 | |
| Be | 1.6 to 1.8 | |
| Ni | 0.2 to 0.6 | |
| Fe | 0 to 0.4 | |
| Si | 0 to 0.2 | |
| Al | 0 to 0.2 | |
| res. | 0 to 0.5 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B194: Standard Specification for Copper-Beryllium Alloy Plate, Sheet, Strip, and Rolled Bar
Copper Alloys: Preparation, Properties and Applications, Michael Naboka and Jennifer Giordano (editors), 2013
ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001
CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015