Annealed (+A) 1.0308 Steel
EN 1.0308 +A steel is EN 1.0308 steel in the annealed condition. It has the lowest strength compared to the other variants of EN 1.0308 steel. The graph bars on the material properties cards below compare EN 1.0308 +A steel to: wrought carbon or non-alloy steels (top), all iron alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Brinell Hardness
100
Elastic (Young's, Tensile) Modulus
190 GPa 27 x 106 psi
Elongation at Break
28 %
Fatigue Strength
140 MPa 20 x 103 psi
Poisson's Ratio
0.29
Shear Modulus
73 GPa 11 x 106 psi
Shear Strength
230 MPa 34 x 103 psi
Tensile Strength: Ultimate (UTS)
360 MPa 52 x 103 psi
Tensile Strength: Yield (Proof)
190 MPa 27 x 103 psi
Thermal Properties
Latent Heat of Fusion
250 J/g
Maximum Temperature: Mechanical
400 °C 750 °F
Melting Completion (Liquidus)
1460 °C 2670 °F
Melting Onset (Solidus)
1420 °C 2590 °F
Specific Heat Capacity
470 J/kg-K 0.11 BTU/lb-°F
Thermal Conductivity
51 W/m-K 29 BTU/h-ft-°F
Thermal Expansion
12 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
7.1 % IACS
Electrical Conductivity: Equal Weight (Specific)
8.1 % IACS
Otherwise Unclassified Properties
Base Metal Price
1.8 % relative
Density
7.9 g/cm3 490 lb/ft3
Embodied Carbon
1.4 kg CO2/kg material
Embodied Energy
18 MJ/kg 7.9 x 103 BTU/lb
Embodied Water
46 L/kg 5.5 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
85 MJ/m3
Resilience: Unit (Modulus of Resilience)
93 kJ/m3
Stiffness to Weight: Axial
13 points
Stiffness to Weight: Bending
24 points
Strength to Weight: Axial
13 points
Strength to Weight: Bending
14 points
Thermal Diffusivity
14 mm2/s
Thermal Shock Resistance
11 points
Alloy Composition
| Fe | 98.2 to 100 | |
| Mn | 0 to 1.2 | |
| Si | 0 to 0.35 | |
| C | 0 to 0.17 | |
| P | 0 to 0.045 | |
| S | 0 to 0.045 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
EN 10296-1: Welded circular steel tubes for mechanical and general engineering purposes - Technical delivery conditions - Part 1: Non-alloy and alloy steel tubes
Microstructure of Steels and Cast Irons, Madeleine Durand-Charre, 2004
Carbon Steel Handbook, D. Gandy, 2007
Ferrous Materials: Steel and Cast Iron, Hans Berns and Werner Theisen, 2008
CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015
Steels: Processing, Structure, and Performance, 2nd ed., George Krauss, 2015