Half-Hard (H02) C19200 Copper
H02 C19200 copper is C19200 copper in the H02 (half hard) temper. The graph bars on the material properties cards below compare H02 C19200 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
120 GPa 17 x 106 psi
Elongation at Break
18 %
Poisson's Ratio
0.34
Rockwell B Hardness
58
Rockwell Superficial 30T Hardness
60
Shear Modulus
44 GPa 6.3 x 106 psi
Shear Strength
260 MPa 38 x 103 psi
Tensile Strength: Ultimate (UTS)
420 MPa 61 x 103 psi
Tensile Strength: Yield (Proof)
310 MPa 45 x 103 psi
Thermal Properties
Latent Heat of Fusion
210 J/g
Maximum Temperature: Mechanical
200 °C 390 °F
Melting Completion (Liquidus)
1080 °C 1980 °F
Melting Onset (Solidus)
1080 °C 1970 °F
Specific Heat Capacity
390 J/kg-K 0.092 BTU/lb-°F
Thermal Conductivity
240 W/m-K 140 BTU/h-ft-°F
Thermal Expansion
17 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
67 % IACS
Electrical Conductivity: Equal Weight (Specific)
68 % IACS
Otherwise Unclassified Properties
Base Metal Price
30 % relative
Density
8.9 g/cm3 560 lb/ft3
Embodied Carbon
2.6 kg CO2/kg material
Embodied Energy
41 MJ/kg 18 x 103 BTU/lb
Embodied Water
310 L/kg 37 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
69 MJ/m3
Resilience: Unit (Modulus of Resilience)
410 kJ/m3
Stiffness to Weight: Axial
7.2 points
Stiffness to Weight: Bending
18 points
Strength to Weight: Axial
13 points
Strength to Weight: Bending
14 points
Thermal Diffusivity
69 mm2/s
Thermal Shock Resistance
15 points
Alloy Composition
| Cu | 98.5 to 99.19 | |
| Fe | 0.8 to 1.2 | |
| Zn | 0 to 0.2 | |
| P | 0.010 to 0.040 | |
| Pb | 0 to 0.030 | |
| res. | 0 to 0.2 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B465: Standard Specification for Copper-Iron Alloy Plate, Sheet, Strip, and Rolled Bar