Half-Hard (H02) C34500 Brass
H02 C34500 brass is C34500 brass in the H02 (half hard) temper. It has the highest strength and lowest ductility compared to the other variants of C34500 brass. The graph bars on the material properties cards below compare H02 C34500 brass to: wrought brasses (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.
Mechanical Properties
Elastic (Young's, Tensile) Modulus
100 GPa 15 x 106 psi
Elongation at Break
12 %
Poisson's Ratio
0.31
Shear Modulus
40 GPa 5.7 x 106 psi
Shear Strength
260 MPa 38 x 103 psi
Tensile Strength: Ultimate (UTS)
430 MPa 62 x 103 psi
Tensile Strength: Yield (Proof)
180 MPa 26 x 103 psi
Thermal Properties
Latent Heat of Fusion
170 J/g
Maximum Temperature: Mechanical
120 °C 250 °F
Melting Completion (Liquidus)
910 °C 1670 °F
Melting Onset (Solidus)
890 °C 1630 °F
Specific Heat Capacity
380 J/kg-K 0.091 BTU/lb-°F
Thermal Conductivity
120 W/m-K 67 BTU/h-ft-°F
Thermal Expansion
21 µm/m-K
Electrical Properties
Electrical Conductivity: Equal Volume
26 % IACS
Electrical Conductivity: Equal Weight (Specific)
29 % IACS
Otherwise Unclassified Properties
Base Metal Price
24 % relative
Density
8.2 g/cm3 510 lb/ft3
Embodied Carbon
2.6 kg CO2/kg material
Embodied Energy
45 MJ/kg 19 x 103 BTU/lb
Embodied Water
320 L/kg 38 gal/lb
Common Calculations
Resilience: Ultimate (Unit Rupture Work)
42 MJ/m3
Resilience: Unit (Modulus of Resilience)
160 kJ/m3
Stiffness to Weight: Axial
7.1 points
Stiffness to Weight: Bending
19 points
Strength to Weight: Axial
15 points
Strength to Weight: Bending
16 points
Thermal Diffusivity
37 mm2/s
Thermal Shock Resistance
14 points
Alloy Composition
| Cu | 62 to 65 | |
| Zn | 32 to 36.5 | |
| Pb | 1.5 to 2.5 | |
| Fe | 0 to 0.15 | |
| res. | 0 to 0.4 |
All values are % weight. Ranges represent what is permitted under applicable standards.
Followup Questions
Further Reading
ASTM B453: Standard Specification for Copper-Zinc-Lead Alloy (Leaded-Brass) Rod, Bar, and Shapes
ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001