MakeItFrom.com
Menu (ESC)

EN 1.4021 (X20Cr13) Stainless Steel

EN 1.4021 stainless steel is a martensitic stainless steel formulated for primary forming into wrought products. 1.4021 is the EN numeric designation for this material. X20Cr13 is the EN chemical designation.

It has a moderately low embodied energy among the wrought martensitic stainless steels in the database.

The properties of EN 1.4021 stainless steel include five common variations. This page shows summary ranges across all of them. For more specific values, follow the links immediately below. The graph bars on the material properties cards further below compare EN 1.4021 stainless steel to: wrought martensitic stainless steels (top), all iron alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

190 GPa 28 x 106 psi

Elongation at Break

11 to 17 %

Fatigue Strength

240 to 380 MPa 35 to 56 x 103 psi

Poisson's Ratio

0.28

Shear Modulus

76 GPa 11 x 106 psi

Shear Strength

390 to 530 MPa 57 to 77 x 103 psi

Tensile Strength: Ultimate (UTS)

630 to 880 MPa 92 to 130 x 103 psi

Tensile Strength: Yield (Proof)

390 to 670 MPa 57 to 97 x 103 psi

Thermal Properties

Latent Heat of Fusion

270 J/g

Maximum Temperature: Corrosion

390 °C 730 °F

Maximum Temperature: Mechanical

760 °C 1390 °F

Melting Completion (Liquidus)

1440 °C 2630 °F

Melting Onset (Solidus)

1400 °C 2550 °F

Specific Heat Capacity

480 J/kg-K 0.11 BTU/lb-°F

Thermal Conductivity

30 W/m-K 17 BTU/h-ft-°F

Thermal Expansion

11 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

2.9 % IACS

Electrical Conductivity: Equal Weight (Specific)

3.3 % IACS

Otherwise Unclassified Properties

Base Metal Price

7.0 % relative

Density

7.7 g/cm3 480 lb/ft3

Embodied Carbon

1.9 kg CO2/kg material

Embodied Energy

27 MJ/kg 12 x 103 BTU/lb

Embodied Water

100 L/kg 12 gal/lb

Common Calculations

PREN (Pitting Resistance)

13

Resilience: Ultimate (Unit Rupture Work)

88 to 110 MJ/m3

Resilience: Unit (Modulus of Resilience)

400 to 1160 kJ/m3

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

25 points

Strength to Weight: Axial

23 to 31 points

Strength to Weight: Bending

21 to 26 points

Thermal Diffusivity

8.1 mm2/s

Thermal Shock Resistance

22 to 31 points

Alloy Composition

Among wrought stainless steels, the composition of EN 1.4021 stainless steel is notable for containing comparatively high amounts of chromium (Cr) and manganese (Mn). Chromium is the defining alloying element of stainless steel. Higher chromium content imparts additional corrosion resistance. Manganese is used to improve ductility at elevated temperatures. It also permits a higher nitrogen content than would otherwise be possible.

Iron (Fe) 83.2 to 87.8
Chromium (Cr) 12 to 14
Manganese (Mn) 0 to 1.5
Silicon (Si) 0 to 1.0
Carbon (C) 0.16 to 0.25
Phosphorus (P) 0 to 0.040
Sulfur (S) 0 to 0.015

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Similar Alloys

Further Reading

EN 10250-4: Open die steel forgings for general engineering purposes - Part 4: Stainless steels

EN 10088-2: Stainless steels - Part 2: Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes

EN 10088-3: Stainless steels - Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes

EN 10088-1: Stainless steels - Part 1: List of stainless steels

Corrosion of Stainless Steels, A. John Sedriks, 1996